Precipitaion Hardening Stainless Steel
High Temperature Alloy
◆0Cr17Ni7Al is a precipitation-hardening steel with Al added, used as springs, washers, calculator components, etc.
◆0Cr15Ni7Mo2Al is used for high-strength containers, parts and structural parts with certain corrosion resistance requirements.
◆The performance of 0Cr15Ni5Cu4Nb is similar to that of 0Cr17Ni4Cu4Nb, but it has better lateral performance.
◆0Cr12Mn5Ni4Mo3Al (Gangyan 69111) has better plasticity than 0Cr15Ni7Mo2Al.
◆0Cr17Ni4Cu4Nb Precipitation hardening steel with Cu added, widely used in shafts, high-strength structural parts requiring corrosion resistance for steam turbine parts.
◆XM-25 is heat and high temperature resistant, suitable for petroleum, chemical, aerospace, nuclear power and other industries.
Chemical composition
Grade |
C |
Si |
Mn |
S |
P |
Cr |
Ni |
Mo |
Cu |
Nb |
Al |
other |
no greater than |
||||||||||||
0Cr17Ni4Cu4Nb |
0.07 |
1 |
1 |
0.035 |
0.03 |
15.5~17.5 |
3~5 |
- |
3~5 |
0.15~0.45 |
- |
- |
0Cr17Ni7Al |
0.09 |
1 |
1 |
0.035 |
0.03 |
16~18 |
6.5~7.5 |
- |
≤0.5 |
- |
0.75~1.5 |
- |
0Cr15Ni7Mo2Al |
0.09 |
1 |
1 |
0.035 |
0.03 |
14~16 |
6.5~7.75 |
2~3 |
- |
- |
0.75~1.5 |
- |
0Cr15Ni5Cu4Nb |
0.07 |
1 |
1 |
0.035 |
0.03 |
14~15.5 |
3.5~5.5 |
- |
2.5~4.5 |
5*C%~0.45 |
- |
- |
0Cr12Mn5Ni4Mo3Al |
0.09 |
0.8 |
4.4~5.3 |
0.03 |
0.03 |
11~12 |
4~5 |
2.7~3.3 |
- |
- |
0.5~1 |
- |
XM-25 |
0.05 |
1 |
1 |
0.03 |
0.03 |
14~16 |
5~7 |
0.5~1 |
1.25~1.75 |
≥8*C% |
- |
- |
Alloy property minimum
Grade |
state |
tensile strength RmN/m㎡ |
Yield Strength Rp0.2N/m㎡ |
Elongation As% |
HRC(HBS) |
0Cr17Ni7Al |
solid solution 1000~1100℃fast cooling |
≤1030 |
≤380 |
≥20 |
≤229 |
565℃aging |
≥1140 |
≥960 |
≥5 |
≥363 |
|
510℃aging |
≥1230 |
≥1030 |
≥4 |
≥388 |
|
0Cr17Ni4Cu4Nb |
480℃aging |
≥1310 |
≥1180 |
≥10 |
≥40 |
550℃aging |
≥1060 |
≥1000 |
≥12 |
≥35 |
|
580℃aging |
≥1000 |
≥865 |
≥13 |
≥31 |
|
620℃aging |
≥930 |
≥325 |
≥16 |
≥28 |
|
0Cr15Ni5Cu4Nb |
solid solution |
- |
- |
- |
≤380 |
565℃aging |
≥1210 |
≥1100 |
≥7 |
≥375 |
|
510℃aging |
≥1320 |
≥1210 |
≥6 |
≥388 |
|
0Cr12Mn5Ni4Mo3Al |
520℃aging |
≥1520 |
≥1280 |
≥9 |
≥47 |
XM-25 |
560℃aging |
≥1100 |
≥1000 |
≥10 |
≥45 |